When inspecting rust and cracks in the weld seams of an excavator boom side plate, the paint and rust on the weld surface should be scraped off or ground clean. During observation, gently tap the weld seam with a small hammer; a magnifying glass can be used if necessary.
1. Causes of Cracks
The causes of cracks in the excavator boom side plate include: air bubbles, slag inclusions, and micro-cracks in the original weld seam. When the excavator is overloaded, these micro-cracks will appear at the original weld seam and slowly expand; the welding rod and the plate material properties may not be compatible, resulting in cracks; due to the large size of the excavator boom, reliable and effective heating and insulation measures are difficult to implement, and the hardened area of the base material around the weld seam may not be completely removed after welding, leading to a decrease in weld strength; the large vibrations and impacts during excavator operation cause uneven stress at the weld seam, leading to cracking.
2. Repair Methods
Pre-welding preparation: Use a hand grinder to clean the oil, paint, rust, etc., from the original weld seam crack. Use an air gouger to cut away the weld seam crack down to the main body of the side plate, and clean away the hardened area of the base material from previous welding. After planing, use an angle grinder to smooth the cut surface (grind a V-shaped bevel on the inner interface). After cleaning and inspection, confirm that all cracks have been located and removed.
Based on the existing repair conditions, select Φ5mm E5015 (J507) or E5016 (J506) welding rods. Bake at 350℃ for 2 hours, then maintain at 100℃ to prevent moisture absorption. Use as needed. Welding current: 190–230A. Due to the large thickness of the excavator side plates, preheat the welding area to 150–250℃ before welding. During welding, use segmented, symmetrical, and backward welding methods. During weld cooling, continuously tap the weld metal with a hand hammer to relieve stress. When welding at the corners of the side plates, to avoid arc defects, continuous welding is recommended to improve the stress condition at the joint.
After welding, thoroughly remove spatter, slag, and weld beads. The weld reinforcement should not exceed 2.5mm. Perform magnetic particle testing on the weld; cracks and other defects are not permitted.
3. Measures to Prevent Weld Corrosion
Thoroughly grind, remove rust from the weld, and apply rust-preventive paint. At the excavation site, for existing rusted welds, manual rust removal can be chosen depending on the actual situation. The disadvantage is that it requires significant labor intensity and is costly. Alternatively, acid pickling can be used. This involves using organic acids as the main base, combined with corrosion inhibitors, surfactants, rust removers, rust inhibitors, and film-forming agents to create an acid pickling solution with rust removal, rust prevention, and primer functions. The cleaning process achieves both rust removal and rust prevention.
Furthermore, during use, ensure the excavator is kept in a clean and dry environment with good ventilation to promptly remove corrosive gases and moisture.